Grade : | АMg5 ( АМг5 ) ( 1550 ) |
Classification : | Aluminium wrought alloys |
Equivalent grades: | Go here |
Fe | Si | Mn | Ti | Al | Cu | Be | Mg | Zn | Impurity |
---|---|---|---|---|---|---|---|---|---|
max 0.5 | 0.3 - 0.8 | 0.02 - 0.1 | 91.9 - 94.68 | max 0.1 | 0.0002 - 0.005 | 4.8 - 5.8 | max 0.2 | other, each 0.05; all 0.1 |
Mechanical properties under T=20°C for grade AMg5 (AMr5) | ||||||||
---|---|---|---|---|---|---|---|---|
Assortment | Dimension (mm) | Direct. | σB (MPa) | σT (MPa) | δ (%) | ψ (%) | KCU (kJ/m²) | Heat treatment |
Pipe, GOST 18482-79 | - | - | 255 | 110 | 15 | - | - | - |
Bar, GOST 21488-97 | - | - | 245-265 | 110-120 | 10-15 | - | - | - |
Band, GOST 13726-97 | - | - | 275 | 130 | 12-15 | - | - | - |
Profile, GOST 8617-81 | - | - | 255 | 175 | 15 | - | - | - |
Plate , GOST 17232-99 | - | - | 255-265 | 110-120 | 12-13 | - | - | - |
Brinell hardness for AMg5 (AMr5), HB 10 -1 = 45 MPa |
Brinell hardness for AMg5 (AMr5) (cold-worked), HB 10 -1 = 60 MPa |
Weldability: without limitations. |
T | E 10⁵ | α 10⁶ | λ | ρ | C | R 10⁹ |
---|---|---|---|---|---|---|
Grade | MPa | 1/Grade | Watt/(m·Grade) | kg/m³ | J/(kg·Grade) | Ohm·m |
20 | 2660 | 49.6 | ||||
100 | 126 | 922 |
Warning! Indicated both exact and nearest equivalents.
USA | Germany | Japan |
---|---|---|
- | DIN, WNr | JIS |
AA5056 | 3.3555 AlMg5 | 5056 |
B51 - Non-ferrous metals, including rare metals, and their alloys
B52 - Graded and shaped rolling
B53 - Sheets and Strips
B54 - Ribbons
B55 - Bars
B64 - Pipes of non-ferrous metals and alloys
σB - Tensile strength [MPa]
σT - Yield stress [MPa]
δ5 - Specific elongation at fracture [%]
ψ - Reduction of area [%]
KCU - Impact strength [kJ/m²]
HB - Brinell hardness [MPa]
T - Test temperature [Grade]
E - Young modulus [MPa]
α - Coefficient of linear expansion (20° - T) [1/Grade]
λ - Thermal (heat) condition coefficient [Watt/(m·Grade)]
ρ - Density [kg/m³]
C - Specific heat (range 20° - T) [J/(kg·Grade)]
R - Electrical resistance [Ohm·m]